                      3.1.2.   Charpy test

                                       Table 3.1.2 Result of charpy impact test.
            Ratio Sample                                Energy Absorb

                               Sample          Angle (º)        Charpy (J)           Average
                80:20        Sample 1.1           110              5.32                5.50

                             Sample 1.2           109              5.87
                             Sample 1.3           110              5.32

                60:40        Sample 2.1           107              6.99                7.18
                             Sample 2.2           106              7.55

                             Sample 2.3           107              6.99
                50:50        Sample 3.1           106              7.55                7.56

                             Sample 3.2           109              5.87
                             Sample 3.3           103              9.26


                        Based on the data and information above, shows the energy absorbed for the impact test (charpy) on all
                 samples  used.  The  charpy  test  used  is  to  determine  the  amount  of  energy  absorbed  by  the  material  during
                 fracture. The value of the charpy has different values on all the different samples which it is based on the angle
                 that was obtained when performing the test. The results of the study found that the highest maximum average
                 charpy is 7.56J that is in the sample 3 (50:50). This indicates that the sample has a lot of energy absorbed by the
                 material compared to other samples. Sample 2 (60:40) has an energy absorb of 7.18J. Meanwhile, the minimum
                 average energy absorb is 5.50J on sample 1 (80:20). The amount of energy absorbed can determine the strength
                 and position of the material depending on the ductile-brittle transition. It is widely used in industry, as it is easy
                 to carry out and results can be obtained quickly.


             4.  Physical testing on mangrove polymer composite

                 For physical testing, only water absorption test conducted. The sample of ratio used is (epoxy: fiber)

                          Sample 1 (80:20)

                          Sample 2 (60:40)

                          Sample 3 (50:50)












          183 | O M I I C O T - V O L 2 1