Page 85 - Batk-Semester-1 kls 10
P. 85
Tabel 1 - 8 Perlakuan pada AluminiumPaduan
Mampu Persentase elemen paduan – aluminium
Paduan diperlaku
kan Copper Silicon Manga Magnesi Zinc chrom
panas nese um
1100 N - - - - - -
3003 N - - 1.2 - - -
2017 H .0 - 0.5 0.5 - -
2117 H 2.5 - - 0.3 - -
2024 H 4.5 - 0.6 1.5 - -
5052 N - - - 2.5 - 0.25
6061 H 0.25 0.6 - 1.0 - 0.25
7075 H 1.6 - - 2.5 5.6 0.3
N = Non Heat treatable
H = Heat treatable
Tabel 1 - 9 Larutan & Mempercepat Perlakuan Panas (Solution & Precipittion Heat Treatment)
Mempercepat perlakuan
Perlakuan panas dlm larutan
panas
Paduan Perenca Perencana Waktu Peren
0
Suhu F Pendingin naan an suhu penuaan canaan
suhu suhu
2017 390 - 950 Air dingin - - T
2117 30 - 950 Air dingin T4 - - T
2024 910 - 930 Air dingin T4 - - T
6061 960 - 980 Air T4 315-325 18 jam T6
atau -
T4 345 - 355 8 jam T6
7075 870 Air 250 24 jam T6
BATK Sem 1 60