 18:54:00  Ground floor  First floor  Second floor  45.67 min  Two glass panels fall out intact. 1 MDF sheet burns and falls

 -12 min  Data acquisition begins  46.83 min  Another set of glass and MDF panels fall. Temp reaches around 1186°C (>660°C)
                                                                                                      Flames begin to leap out from ground
 -10.75 min  Fire load in plastic basket near crib is manually ignited  48 min  Flashover occurs during this interval. Temperatures reached around 1200°C  floor. Temp at first floor level is about 735°C


 0 min  Re-ignition of fuel source with extra waste papers is attempted                            Fire did not propagate to first floor and failed
               55.75 min       Fire load is consumed and fire begins to die out. Temp reduce to 620°C  to ignite MDF panels (i.e. no leap-frog observed
                                                                                                            from ground to first floor)
 Wooden crib placed near ignition source ignites.
 2 min  TC at base level shows max temp of 60°C whereas TC at roof level   59.25 min                  Ignition of wooden crib using gasoline
 above crib shows temp of 275°C. Temp beneath cement board is about 23°C


 29 min  Wooden crib is consumed and fails to ignite the components within  66 min                        IMDF panel begins to shrink.
 the compartment. Video camera stops functioning                                                          Temperature is around 550°C
                                                                                                     MDF panel catches fire. Glass panel has
 33 min  Ignition with gasoline is attempted
               67.25 min                                                                               fallen intact due to failure of binder.
                                                                                                           Temp reach around 850°C
 35 min  Cement boards are intact. Max temp observed is around 475°C                                   Flashover occurs during this interval.
                69 min
                                                                                                    Temperature increased to 1050°C (>660°C)
 36.47 min  Cement board placed above wooden crib fall.
 Max temp at this instant is around 630°C                                                              All glass and MDF panels have fallen.
               70.33 min                                                                                 Aluminium cladding framework
                                                                                                         has melted at several locations
 41 min  MDF panel begins to shrink. Temp reaches about 685°C
                                                                                                       Fire begins to die out. Minor failure    Second floor does
               74.33 min                                                                                  of cement boards is observed            not catch fire
 Glass panel falls in intact form due to failure of binder.
 44.67 min  Max temp is about 755°C. Unlike ACP, MDF was not easily catching fire  75.17 min  Fire extinguishing begins  Fire extinguishing begins  Fire extinguishing begins