PENGUJIAN BAHAN 2 (BETON ASPAL)


                       Contoh Hasil Uji Marshall dengan Filler Semen 5% (Wiyono,  Susilowati, 2018)
                                                                      %
                                                         Kadar Aspal ( )
                         Sifat Campuran                                                    Ket
                                             5        5.5       6       6.5        7
                          % Rongga Thd     20.51     20.14    18.51    19.16     18.43   min 15
                         Agregat (VMA)
                         % Rongga Terisi   52.10     59.29    71.88    75.79     88.83   min 65
                          Aspal (VFB)
                          % Rongga Thd      9.83     8.21      5.26     4.66     2.04    3.5-5.5
                        Campuran (VIM)
                            Stabilitas                                                     min
                                          1337.74  1361.22  1432.78  1483.67  1936.67
                                                                                           800
                            Kelelehan                                                     2 - 4
                                            4.53     4.87      5.10     4.70     5.10
                                                                                           mm
                            Marshall       257.09   274.12    293.06   319.29   401.81     min
                            Quotient                                                       250